SA387 Steel Plate

SA387 Steel Plate, Grades 5, 9, 11, 12, 22 and 91 Class 1 and 2
Chromium – Molybdenum Alloy Steel Plates for elevated temp + corrosion. For Use in Boilers and pressure vessels.

Chemical Properties:

SA387/ASTM A387

Grade 5

Grade 9

Grade 11

Grade 12

Grade 22

Carbon

0.15 max

0.15 max

0.04 – 0.17

0.04 – 0.17

0.04 – 0.15

Manganese

0.25 – 0.66

0.25 – 0.66

0.35 – 0.73

0.35 – 0.73

0.25 – 0.66

Phosphorous

0.035

0.030

0.035

0.035

0.035

Sulfur

0.030

0.030

0.035

0.035

0.035

Silicon

0.55 max

1.05 max

0.44 – 0.86

0.13 – 0.45

0.5 max

Chromium

3.9 – 6.1

7.9 – 10.1

0.94 – 1.56

0.74 – 1.21

1.88 – 2.62

Molybdenum

0.40 – 0.7

0.85 1.15

0.40 – 0.7

0.4 – 0.65

0.85 – 1.15

SA387/ASTM A387 GR 5 CLASS 2

A high quality chrome molybdenum alloy steel plate intended specifically for use in weldable carbon steel pressure vessels at elevated temperatures. Added molybdenum gives the material greater temperature tensile strength and the chromium provides improved corrosion resistance.

SA387/ASTM A387 GR 9 CLASS 2

Weldable carbon steel plates for pressure vessels and boilers used in elevated temperatures. The material benefits from added chromium and molybdenum which gives the steel greater corrosion resistance and resistance to heat. SA387 Grade 9 is used by fabricators who serve the oil, gas and petrochemical industry.

SA387/ASTM A387 GR 11 CLASS 2

A pressure vessel grade steel for use in elevated temperature service, ASME SA387 Grade 11 Class 2 is used in a variety of industries and is highly effective, particularly in the oil, gas and petrochemical industry, where liquids and gases are often stored at higher temperatures.

The higher levels of chromium also provide excellent corrosion and oxidation resistance, which is a must in sour gas applications.

SA387/ASTM A387 GR 12 CLASS 2

Engineered for use in elevated temperature service, ASME SA387 Grade 12 is a chrome molybdenum carbon alloy steel for use in weldable pressure vessels and industrial boilers.
The material benefits from added chromium which provides excellent corrosion and oxidation resistance making it ideal for sour service applications in the oil and gas industry.

SA387/ASTM A387 GR 22 CLASS 2

We supply ASME SA387 Grade 22 Class 2 plates to fabricators serving the oil, gas and petrochemical industry. These industries require a pressure vessel grade steel which works well in elevated temperatures and our material serves this purpose well. And with good corrosion and oxidation resistance, SA387 Grade 22 Class 2 plates are a good option.

SA387/ASTM A387 GR 91 CLASS 2

Where resistance to high temperature and good anti-corrosion characteristics are required, ASME SA387 Grade 91 Class 2 carbon alloy steel plate is a material to consider. It is a pressure vessel grade steel which is used commonly by fabricators who supply the oil and gas industry.

Due to the materials excellent corrosion resistant properties, SA387 Grade 91 is also an option for use in sour service environments. The material has good weldability and with its heat resistant qualities, the material is a highly versatile steel which can be used in numerous applications.

ASTM A387/ SA387

Pressure Vessel Plates, Alloy Steel, Chromium-Molybdenum
IN STOCK FOR IMMEDIATE SHIPMENT

Mechanical Properties:

A 387 Grade 5

A 387 Grade 9

A 387 Grade 11

A 387 Grade 12

A 387 Grade 22

Class 1

Class 2

Class 1

Class 2

Class 1

Class 2

Class 1

Class 2

Class 1

Class 2

Tensile

60-85

75-100

60-85

75-100

60-85

70-90

50-80

65-85

60-85

75-100

Strength (ksi)

Tensile

415-585

515-690

415-585

515-690

415-585

485-620

380-550

450-585

415-585

515-690

Strength (MPa)

Yield

30

45

30

45

35

45

33

40

30

45

Strength (ksi)

Yield

205

310

205

310

240

310

230

275

205

310

Strength (MPa)

Elongation

19

18

18

19

in 200mm (%)

Elongation

18

18

18

18

22

22

22

22

18

18

in 50mm (%)

Reduction of

45

45

45

45

45

45

area in %

Chemical Properties:

Grade 5

Grade 9

Grade 11

Grade 12

Grade 22

Carbon

Heat Analysis

0.15 max

0.15 max

0.05 – 0.17

0.05 – 0.17

0.05 – 0.15

Product Analysis

0.15 max

0.15 max

0.04 – 0.17

0.04 – 0.17

0.04 – 0.15

Manganese

Heat Analysis

0.3 – 0.6

0.30 – 0.6

0.4 – 0.65

0.4 – 0.65

0.3 – 0.6

Product Analysis

0.25 – 0.66

0.25 – 0.66

0.35 – 0.73

0.35 – 0.73

0.25 – 0.66

Phosphorous

Heat Analysis

0.035

0.03

0.035

0.035

0.035

Product Analysis

0.035

0.03

0.035

0.035

0.035

Sulphur

Heat Analysis

0.03

0.03

0.035

0.035

0.035

Product Analysis

0.03

0.03

0.035

0.035

0.035

Silicon

Heat Analysis

0.5 max

1.0 max

0.5 – 0.80

0.15 – 0.4

0.5 max

Product Analysis

0.55 max

1.05 max

0.44 – 0.86

0.13 – 0.45

0.5 max

Chromium

Heat Analysis

4.00 – 6.00

8.0 – 10.0

1.0 – 1.5

0.8 – 1.15

2.0 – 2.5

Product Analysis

3.9 – 6.1

7.9 – 10.1

0.94 – 1.56

0.74 – 1.21

1.88 – 2.62

Molybdenum

Heat Analysis

0.45 – 0.65

0.9 – 1.1

0.45 – 0.65

0.45 – 0.6

0.9 – 1.1

Product Analysis

0.40 – 0.7

0.85 1.15

0.40 – 0.7

0.4 – 0.65

0.85 – 1.15

 

  • ASTM A182 Grades F5, F11, F22, F91 Round Bar